Full argon arc welding and argon arc welding bottoming in the process there is no difference, the full argon arc welding for thin-walled small diameter pipe (generally DN60 and below, wall thickness of 4mm) below, the purpose of ensuring that the root of the weld quality of the appearance of the weld forming a good.
When the pipe diameter is larger, wall thickness should be used when the bottom of argon arc welding manual welding cover, with manual welding cover the purpose of the pipe diameter is large with manual welding can ensure the appearance of quality and efficiency is higher than argon arc welding, lower cost than argon arc welding.
Argon arc welding welding process in the boiler water-cooled wall, superheater, economizer, etc. Welding, joint quality is excellent, by ray flaw detection, weld level are in the Ⅱ level or more.



Advantages of argon arc welding bottoming
(1) good quality
As long as you choose the right wire, welding process parameters and good gas protection can make the root to get good penetration, and uniformity of penetration, smooth and neat surface. There is no general electrode arc welding prone to weld tumor, not welded through, depression, porosity and slag and other defects.
(2)High efficiency
In the first layer of pipeline welding, manual argon arc welding is continuous arc welding. And electrode arc welding for the broken arc welding, so manual argon arc welding can improve the efficiency of 2 ~ 4 times. Because the argon arc welding will not produce slag, so no need to clean up the slag and repair the weld channel, the speed to improve faster. In the second layer of arc welding cover, smooth and neat argon arc welding bottoming layer is very conducive to arc welding cover, can ensure good fusion between the layers, especially in the welding of small diameter pipe, the efficiency is more significant.
(3) easy to grasp
Manual electric arc welding root weld, must be experienced and higher technical level of the welder to serve. The use of manual argon arc welding bottom, generally engaged in welding workers after a short period of practice, basically can master.
(4) small deformation
Argon arc welding bottoming heat-affected zone is much smaller, so the deformation of the welded joint is small, residual stress is small.
Introduction to the process
(1)Welding examples
Coal economizer, evaporation section tube bundle, water-cooled wall and low-temperature superheater material for the 20 steel, high-temperature superheater tube for 12Cr1MoV.
(2)Welding preparation
Before welding, the pipe mouth should be made 30 ° bevel, inside and outside the pipe end of 15 mm range should be polished out of the metal color. Pipe counter gap is 1~3mm. when the actual counter gap is too large, need to be first in the pipe bevel side of the pile welding transition layer. Build temporary wind facilities, strictly control the wind speed at the welding operation, because the wind speed exceeds a certain range, it is very easy to produce porosity.
(3)Operation
The use of manual tungsten argon arc welding machine, the welding machine itself is equipped with a high frequency arc-inducing device, you can use high frequency arc-inducing. Arc quenching and electrode arc welding is different, such as arc quenching too fast, it is easy to produce arc crater cracks, so the operation should be led to the edge of the molten pool or the base material is thicker, and then gradually reduce the molten pool slowly arc quenching, and finally shut down the protective gas.
For wall thickness of 3 ~ 4mm 20 steel pipe material, filler material available TIGJ50 (12Cr1 MoV, available 08CrMoV), tungsten electrode rod diameter 2mm, welding current 75 ~ 100A, arc voltage 12 ~ 14V, protective gas flow rate of 8 ~ 10L/min, power supply type for DC positive connection.