Titanium is characterized by low density, high specific strength, corrosion resistance, high elasticity, low damping, non-magnetic and good performance in high and low temperatures, etc. It is known as "space metal" and "ocean metal", and is widely used in the fields of aerospace, seawater desalination, shipbuilding, chemical industry, automobile, electric power and many other fields of national economy and national defense construction. It is widely used in aerospace, seawater desalination, shipbuilding, chemical industry, automobile, electric power and many other national economy and national defense construction fields. Due to the low yield of seamless pipe, long production cycle, high cost, and pure titanium welded pipe production process is short, low production costs, high production efficiency, vigorously develop thin-walled welded pipe has become a trend in today's pipe production. In Japan, Europe and the United States, titanium and titanium alloy thin-walled seamless tubing is gradually replaced by titanium welded tubes, used in coastal power stations and nuclear power plants in the condenser and condenser, not only improve the heat exchange efficiency, but also improve the service life of the condenser and condenser unit, the economic benefits are significant.



Titanium tube welding must be ensured:
(1) The metal in the welding zone above 250 ℃ from the active gas N, 0, H and harmful impurity elements C, Fe, Mn and other pollution.
(2) can not form a coarse crystal organization.
(3) Can not produce large welding residual stress and residual deformation. Therefore, the welding process shall be in accordance with the intended construction sequence, in strict accordance with the process quality management standards, the implementation of the whole process of quality control. So that people, machines, materials, law factors are in a good state of control, so that in a reasonable period of time, to ensure the welding quality of titanium tubes.
Titanium welded pipe burst pressure of 61.76MPa, titanium welded pipe longitudinal weld appeared in a small crack, the pipe water from the weld burst rushed out. Seamless titanium tube: burst pressure of 68.10MPa, the tube test fitting plug connection appeared larger cracks, water from the tube and plug connection burst out of the seamless tube itself did not occur damage. Titanium tube heat exchanger, condenser, condenser, etc. in the process of use by the shell process fluid-induced vibration, caused by different fluid vortex, jitter vibration, elastic excitation and acoustic resonance, the combination of these oscillations to form a violent vibration, which led to the tube constantly impact on the refractory plate, resulting in the tube by the refractory edge of the plate to cut through the tube and the tube and tube plate connection was pulled apart to the occurrence of leaks and other phenomena. Therefore, the titanium welded pipe and titanium seamless pipe fatigue vibration test, statistics in the same conditions of titanium welded pipe and titanium seamless pipe fatigue times, in order to determine the use of titanium welded pipe instead of titanium seamless pipe to determine whether or not the service life of the equipment has an impact.
(1) welded titanium tube expansion: the same expansion pressure, welded titanium tube pull-off force than the seamless titanium tube pull-off force of 2.5-3.1MPa, welded titanium tube expansion and expansion of the tooling combined more closely, expansion of better airtight.
(2) Welded titanium tube can withstand the highest design pressure of 35MPa within the definition of the pressure vessel, holding pressure for 3min without leakage.
(3) Titanium welded pipe and titanium seamless pipe at a frequency of 30.
Welded titanium tube for roll up the principle and process is the same as the titanium seamless tube. However, the presence of welding beads requires the consideration of additional factors in order to determine the best and stable roll-up process. Of these factors, the most important are the metallurgical quality and surface condition of the tube. For example, it is desirable to anneal the tube rather than weld it, for the tube plate design of the tight fit connection must be avoided excessively protruding filler weld beads, it has been proved that the air annealed head with a polished halo of the flared tube bonding strength than in the bright annealed or bright stress relieved annealed state of the tube flared up a little better.
On the other hand, rough tube surfaces or tube plate surfaces improve mechanical strength, but sealing is poor. The use of precision machining or machining plus reamed tube plate hole method of manufacturing titanium tube plate hole surface finish of 0.75-1.5-101, tube head polishing ring finish also reaches the same level, so that the strength and sealing will be able to achieve the best fit.