About heat treatment of white copper
1. Introduction to white copper
Copper-nickel alloys containing Ni <50% (wt) are called white copper.
Since the two elements copper and nickel are very close in the periodic table, their electrochemical properties and atomic radii are not much different, and they are both face-centered cubic lattices, they are infinitely soluble in each other. Copper is non-magnetic and nickel is ferromagnetic. In Cu-Ni binary alloy, as the Ni content decreases, the Curie point of the alloy decreases. When the nickel content drops to 74%, the Curie point drops to room temperature; when the nickel content drops to 50%, the Curie point drops to below -200°C.
Adding nickel to copper can significantly improve strength, corrosion resistance, electrical resistance and thermoelectric properties. Industrial copper-nickel alloys are divided into structural white copper and electrical white copper based on different performance characteristics and uses. The copper-nickel binary alloy is called simple white copper. The outstanding characteristics of simple white copper are its high chemical stability in various corrosive media such as seawater, organic acids, and various salt solutions, and its excellent cold and hot processing properties. The white copper grade number is preceded by "B", followed by the nickel content (%). Cupronickel that also contains other elements is called complex cupronickel or special cupronickel.
Cupronickel containing Mn is called manganese cupronickel, also known as constantan, such as BMn40-1.5. Its composition (wt) is 40% Ni and 1.5% Mn.
Adding a small amount of manganese or iron to white copper can not only refine the grain size, but also significantly improve its corrosion resistance. Therefore, the iron-containing complex white copper - iron-white copper BFe30-1-1 and BFe5-1, can be used as parts working in sea-going ships and other strongly corrosive media.
The main role of zinc in copper-nickel alloys is solid solution strengthening and improving corrosion resistance. Zinc-nickel copper contains Ni between 5%-35% (wt) and Zn between 13%-45% (wt). Among them, BZn15-20 is the most widely used. It has high corrosion resistance, good processing performance, beautiful silver white color, small specific gravity, and low cost. Zinc-nickel copper is added with <2% (wt) Pb and Trace amounts of selenium (Se) and tellurium (Te) can improve processability and are suitable for manufacturing precision mechanical parts.
The solubility of aluminum in copper-nickel alloys decreases as the temperature decreases and can be solid solution strengthened. For example, aluminum-nickel copper BAl13-3 and BAl16-1.5 not only have excellent mechanical properties and corrosion resistance, but also have high elasticity and low temperature resistance. At a low temperature of 90K (-183℃), the mechanical properties not only do not decrease, but actually improve improve!
Adding Ti (titanium), Zr (zirconium), Ne (niobium), Mo and other elements to copper-nickel alloys can improve the casting performance of the alloy, improve room temperature mechanical properties and thermoplasticity, and is also beneficial to welding and corrosion resistance.
Listed below are the mechanical properties and uses of white copper for corrosion-resistant structures:
B5
Strip M, tensile strength 220MPa, elongation 32%
Strip Y, tensile strength 400MPa, elongation 10%
Used for ship corrosion-resistant parts.
B19
Strip Y, tensile strength 400MPa, elongation 10%
Strip M, tensile strength 300MPa, elongation 25%
Strip Y, tensile strength 400MPa, elongation 3%
Plate M, tensile strength 300MPa, elongation 30%
Plate Y, tensile strength 400MPa, elongation 3%
It is used for precision instruments, instrument parts, and metal mesh and chemical corrosion-resistant parts that work in steam, freshwater, and seawater.
B30
Strip M, tensile strength 380MPa
Strip Y, tensile strength 550MPa
Plate M, tensile strength 380MPa, elongation 23%
Plate Y, tensile strength 550MPa, elongation 3%
It is used for corrosion-resistant parts working in steam and sea water, and metal pipes and condensing pipes working under high temperature and high pressure.
BMn3-12
Strip M, tensile strength 360MPa, elongation 25%
Plate Y, tensile strength 360MPa, elongation 25%
The purpose is the same as above.
BZn15-20
Strip M, tensile strength 350MPa, elongation 3.5%
Strip Y, tensile strength 550MPa, elongation 1.5%
Strip T, tensile strength 650MPa, elongation 1%
Plate M, tensile strength 350MPa, elongation 3.5%
Strip Y, tensile strength 550MPa, elongation 2%
Plate T, tensile strength 650MPa, elongation 1%
Control rod Y, diameter 5-20mm, tensile strength 450MPa, elongation 5%
Control rod Y, diameter 21-30mm, tensile strength 400MPa, elongation 7%
Control rod Y, diameter 31-40mm, tensile strength 350MPa, elongation 12%
Control rod M, tensile strength 300MPa, elongation 30%
Used in instrument precision machinery parts, industrial utensils, and medical machinery.
BAl6-1.5
Plate, tensile strength 550MPa, elongation 3%
Used to make springs and elastic parts.
2. The main physical properties of commonly used electrical white copper are introduced below.
Simple white copper B0.6
Thermal conductivity λ272w/(m·℃)
Resistivity ρ0.031×10ˉ6Ω·m
Resistance temperature coefficient 0.0028/℃
Simple white copper B16
Linear expansion coefficient α15.3×10ˉ6/℃
Resistivity ρ0.223×10ˉ6Ω·m
Resistance temperature coefficient 0.0028/℃
Manganese copper BMn3-12
Linear expansion coefficient α16.0×10ˉ6/℃
Specific heat c410J/kg·℃
Thermal conductivity λ22w/(m·℃)
Resistivity ρ0.435×10ˉ6Ω·m
Resistance temperature coefficient 0.00003/℃
Constantan BMn40-1.5
Linear expansion coefficient α14.4×10ˉ6/℃
Specific heat c410J/kg·℃
Thermal conductivity λ21w/(m·℃)
Resistivity ρ0.435×10ˉ6Ω·m
Resistance temperature coefficient 0.00002/℃
Test copper BMn43-0.5
Linear expansion coefficient α14.4×10ˉ6/℃
Thermal conductivity λ24w/(m·℃)
Resistivity ρ0.49×10ˉ6Ω·m
Resistance temperature coefficient-0.00014/℃
3. Heat treatment of white copper
Aluminum white copper BAl2-3 can be strengthened by heat treatment. After solid solution at 900℃, cold rolling 50%, and aging at 550℃, the strength can reach 800-1000MPa, and the solid solution state is only 250-350MPa.
The intracrystal segregation of the white copper ingot is serious and homogenization annealing must be carried out. The homogenization annealing system of white copper is as follows:
B19, B30, temperature 100-1050℃, time 3-4h
BMn3-12, temperature 830-870℃, time 2-3h
BMn40-1.5, temperature 1050-1150℃, time 3-4h
BZn15-20, temperature 940-970℃, time 2-3h
Different heat treatment processes of white copper have a great impact on its performance. BMn3-12 used for precision instruments should be stress-relieved and annealed to stabilize the resistance.
BMn40-1.5 working at high temperatures should be short-term annealed at a higher temperature of 750-850℃, water-cooled or air-cooled.
The zinc-nickel copper BZn15-20 used to make elastic components can be annealed at a low temperature of 325-375°C.
The intermediate annealing temperature (℃) of white copper machined parts needs to be appropriately reduced as the effective thickness (mm) decreases, as listed below:
B19, B25
750-780℃ (>5mm) 700-750℃ (15-mm)
620-700℃ (0.5-1mm) 530-620℃ (<0.5mm)
BZn15-20\bmN3-12
700-750℃ (larger than 5mm) 680-730℃ (1-5mm)
600-700℃ (0.5-1mm) 520-600℃ (<0.5mm)
BAl6-1.5, BAl13-3
700-750℃ (>5mm) 700-730 (1-5mm)
580-700℃ (0.5-1mm) 550-600℃ (<0.5mm)
BMn40-1.5
800-850℃ (>5mm) 750-800℃ (1-5mm)
600-750℃ (0.5-1mm) 550-600℃ (<0.5mm)
The annealing temperature of finished copper-nickel rods and wires also varies with the different states of "semi-hard and soft" before annealing, as listed below:
BZn15-20
Bar, semi-hard 400-420℃, soft 650-700℃
Wire Φ0.3-Φ6.0, soft 650-700℃
BMn3-12
Wire Φ0.3-Φ6.0, soft 500-540℃
BMn40-1.5
Wire Φ0.3-Φ0.8, soft 670-680℃
Wire Φ0.85-Φ2.0, soft 690-700℃
Wire Φ2.1-Φ6.0, soft 710-730℃