Gnee Steel (Tianjin) Co., Ltd.

An in-depth analysis of copper in cables. What kind of copper is good?

Apr 09, 2024

An in-depth analysis of copper in cables. What kind of copper is good?

info-133-133Copper Round Tube Pipe Rod 200/250/300mm Length 1-16mm Id 1- 2mm Wall99.9% Pure Copper Metal Plate, Copper Skin, Copper Foil Thickness

Introduction: Due to the different processes for producing copper rods, the oxygen content and appearance of the copper rods produced are different. The copper rods produced by Shangying have an oxygen content of less than 10ppm with proper technology, which is called oxygen-free copper rods; the copper rods produced by continuous casting are hot rolled under protective conditions, and the oxygen content is in the range of 200-500ppm, but sometimes Up to more than 700ppm. Generally, the copper produced by this method has a bright appearance. Low-oxygen copper rods are sometimes called polished rods.

Oxygen-free copper rod

Copper rod is the main raw material in the cable industry. There are two main production methods - continuous casting and rolling and upward continuous casting. There are many production methods for continuous casting and rolling of low-oxygen copper rods. The characteristic is that after the metal is melted in the shaft furnace, the copper liquid passes through the holding furnace, chute, tundish, and enters the closed mold cavity from the pouring pipe. The cooling intensity is used to cool down to form a cast slab, which is then rolled in multiple passes. The produced low-oxygen copper rod has a hot-processed structure. The original casting structure has been broken, and the oxygen content is generally between 200 and 400 ppm. Oxygen-free copper rods are basically produced in China using the upward continuous casting method. After the metal is melted in an induction furnace, it is continuously cast through graphite molds, and then cold rolled or cold worked. The oxygen-free copper rods produced have a cast structure and contain oxygen. The amount is generally below 20ppm. Due to different manufacturing processes, there are great differences in many aspects such as organizational structure, oxygen content distribution, impurity form and distribution, etc.

1. Drawing performance

The drawing performance of copper rods is related to many factors, such as the content of impurities, oxygen content and distribution, process control, etc. The following is an analysis of the drawing performance of copper rods from the above aspects.

1. The influence of melting method on impurities such as S

Continuous casting and rolling to produce copper rods mainly melts the copper rods through the combustion of gas. During the combustion process, through oxidation and volatilization, some impurities can be reduced from entering the copper liquid to a certain extent. Therefore, the continuous casting and rolling method has relatively high raw material requirements. Lower. The upper continuous casting produces oxygen-free copper rods. Since the induction furnace is used for melting, the "patina" and "copper beans" on the surface of the electrolytic copper are basically melted into the liquid copper. The melted S has a great influence on the plasticity of the oxygen-free copper rod and will increase the wire drawing breakage rate.

2. The entry of impurities during the casting process

During the production process, the continuous casting and rolling process requires the transfer of molten copper through holding furnaces, chutes, and tundishes, which is relatively easy to cause the refractory material to peel off. During the rolling process, it needs to pass through the rolls, causing the iron to fall off and causing damage to the copper rods. Cause external inclusions. The rolling in of oxides on and under the skin during hot rolling will have an adverse effect on the drawing of hypoxic rods. The production process of the upward continuous casting method is short. The copper liquid is completed through the submersible flow in the combined furnace, which has little impact on the refractory materials. The crystallization is carried out in the graphite mold, so there are fewer pollution sources and impurities that may be generated in the process. There are fewer opportunities to enter.

O, S, and P are elements that produce compounds with copper. In molten copper, oxygen can partially dissolve, but when copper condenses, oxygen hardly dissolves in copper. The dissolved oxygen in the molten state precipitates as copper = cuprous oxide eutectic and is distributed at the grain boundaries. The emergence of copper-cuprous oxide eutectic significantly reduces the plasticity of copper.

Sulfur can be dissolved in melt copper, but at room temperature, its solubility is reduced to almost zero. It appears at grain boundaries in the form of cuprous sulfide, which will significantly reduce the plasticity of copper.

3. Oxygen distribution patterns and effects in low-oxygen copper rods and oxygen-free copper rods

The oxygen content has a significant impact on the wire drawing performance of low-oxygen copper rods. When the oxygen content increases to the optimal value, the copper rod has the lowest breakage rate. This is because oxygen acts as a scavenger in its reaction with most impurities. Moderate oxygen is also conducive to removing hydrogen from the copper liquid, generating water vapor to overflow, and reducing the formation of pores. The optimal oxygen content provides the best conditions for the wire drawing process.

Distribution of low-oxygen copper rod oxides: In the initial stage of solidification in continuous casting, the heat dissipation rate and uniform cooling are the main factors that determine the copper rod oxide distribution. Uneven cooling will cause essential differences in the internal structure of the copper rod, but in subsequent thermal processing, the columnar crystals will usually be destroyed, making the cuprous oxide particles refined and evenly distributed. A typical situation resulting from the aggregation of oxide particles is central bursting. In addition to the influence of oxide particle distribution, copper rods with smaller oxide particles show better wire drawing characteristics, and larger Cu2O particles easily cause stress concentration points and break.

The oxygen content of oxygen-free copper exceeds the standard, the copper rod becomes brittle, the elongation decreases, the stretched port appears dark red, and the crystal structure is loose. When the oxygen content exceeds 8ppm, the process performance deteriorates, which is manifested in an extremely high rate of rod breakage and wire breakage during casting and drawing. This is because oxygen can form a brittle phase of cuprous oxide with copper, forming a copper-cuprous oxide eutectic, which is distributed on the boundary in a network structure. This brittle phase has high hardness and will separate from the copper body during cold deformation, causing the mechanical properties of the copper rod to decrease and easily causing fracture during subsequent processing. High oxygen content can also cause the conductivity of oxygen-free copper rods to decrease. Therefore, the upward continuous casting process and product quality must be strictly controlled.

4. The influence of hydrogen

In upward continuous casting, the oxygen content is controlled low and the side effects of oxides are greatly reduced, but the influence of hydrogen becomes a more significant problem. There is an equilibrium reaction in the melt after inhalation: H2O(g)=[O]+2[H];

Gas and porosity are formed during the crystallization process when hydrogen precipitates and accumulates from the supersaturated solution. The hydrogen precipitated before crystallization can reduce cuprous oxide to generate water bubbles. Since the characteristic of upward casting is the crystallization of molten copper from top to bottom, the shape of the liquid formed is approximately conical. The gas precipitated before the copper liquid crystallizes is blocked in the solidification structure during the floating process, and pores are formed in the casting rod during crystallization. When the upward gas content is small, the precipitated hydrogen exists at the grain boundaries and forms porosity; when the gas content is high, it gathers into pores. Therefore, pores and porosity are formed by both hydrogen and water vapor.

Hydrogen comes from various process links in the upstream production process, such as the "patina" of the raw material electrolytic copper, the auxiliary material charcoal**, the climate environment**, and the graphite crystallizer is not dry, etc. Therefore, the surface of the copper liquid in the melting furnace should be covered with baked charcoal, and the electrolytic copper should try to remove "patina", "copper beans" and "ears", which is very important to improve the quality of oxygen-free copper rods.

In the continuous casting and rolling process, hydrogen is often controlled by moderately controlling the oxygen content. Cu2O+ H2= 2Cu+ H2O

Since the molten copper crystallizes from the bottom up during the casting process, the water vapor generated by the oxygen and hydrogen in the molten copper can easily float up and escape. Most of the hydrogen in the molten copper can be effectively removed, thus affecting the copper rod. smaller.

goTop