The thermal conductivity of titanium rods and titanium alloy bar blanks is relatively low, and this characteristic is particularly significant in the hot extrusion process. Due to the lack of thermal conductivity, the temperature difference between the surface layer and the inner layer of the billet is extremely large. Especially when the extrusion cylinder temperature is set at 400 degrees, this temperature difference may even reach 200 to 250 degrees. The suction strengthening effect and the temperature difference between the billet sections work together, resulting in a significant difference between the billet surface and the center of the metal in the strength properties and plastic properties. This difference in the extrusion process will lead to uneven deformation, thus generating a large additional tensile stress in the surface layer, which is the main reason for the formation of cracks and cracks on the surface of the extruded products.
The hot extrusion process of titanium rods and titanium alloy rods is more complex than that of aluminum alloys, copper alloys and even steel. This complexity is mainly due to the special physicochemical properties of titanium and titanium alloys. Industrial titanium alloys of metal flow dynamics research shows that in the temperature interval of different phase states, the flow behavior of the metal will appear significant changes. Therefore, the heating temperature of the billet, a key factor in determining the phase state of the metal, has an important influence on the extrusion flow characteristics of titanium rods and titanium alloy bars. Extrusion at α or α+β phase zone temperatures results in more uniform metal flow than extrusion at β phase zone temperatures.
However, obtaining extruded products with high surface quality is a difficult task for titanium alloy bars. Until now, the extrusion of titanium rods has been dependent on the use of lubricants. This is mainly due to the fact that titanium forms fusible eutectic crystals with iron-based or nickel-based alloy die materials at elevated temperatures of 980 and 1030 degrees Celsius, resulting in intense die wear.



The main factors affecting the flow of metal during the extrusion process include:
1. extrusion method reverse extrusion compared to forward extrusion, metal flow is more uniform; cold extrusion compared to hot extrusion, metal flow is also more uniform; lubricated extrusion compared to non-lubricated extrusion, metal flow is also more uniform. These effects are mainly realized by changing the friction conditions.
2. Extrusion speed: with the increase of extrusion speed, the unevenness of metal flow will increase.
3. Extrusion Temperature: As the extrusion temperature increases, the deformation resistance of the billet decreases, but the uneven flow of metal also increases. If the heating temperature of the extrusion barrel and die is too low, the temperature difference between the outer layer and the center layer of the metal increases, and the unevenness of metal flow will also increase. The better the thermal conductivity of the metal, the more uniform the temperature distribution on the end face of the ingot billet.
4. Metal Strength All other things being equal, the higher the metal strength, the more uniform the metal flow.
5. Die angle: The larger the die angle (i.e. the angle between the die end face and the center axis), the more uneven the metal flow. However, when extruding with a perforated die and a reasonable arrangement of die holes, the metal flow will tend to be uniform.
6. The degree of deformation is either too large or too small, resulting in uneven metal flow.
In summary, the characteristics of the hot extrusion process of titanium rods and titanium alloy rods are complex and variable, and a variety of factors need to be considered to ensure the quality and performance of extruded products.